Atomic Layer Deposition of Buffer Layers for the Growth of Vertically Aligned Carbon Nanotube Arrays

Nanoscale Research Letters, Apr 2019

Vertically aligned carbon nanotube arrays (VACNTs) show a great potential for various applications, such as thermal interface materials (TIMs). Besides the thermally oxidized SiO2, atomic layer deposition (ALD) was also used to synthesize oxide buffer layers before the deposition of the catalyst, such as Al2O3, TiO2, and ZnO. The growth of VACNTs was found to be largely dependent on different oxide buffer layers, which generally prevented the diffusion of the catalyst into the substrate. Among them, the thickest and densest VACNTs could be achieved on Al2O3, and carbon nanotubes were mostly triple-walled. Besides, the deposition temperature was critical to the growth of VACNTs on Al2O3, and their growth rate obviously reduced above 650 °C, which might be related to the Ostwald ripening of the catalyst nanoparticles or subsurface diffusion of the catalyst. Furthermore, the VACNTs/graphene composite film was prepared as the thermal interface material. The VACNTs and graphene were proved to be the effective vertical and transverse heat transfer pathways in it, respectively.

A PDF file should load here. If you do not see its contents the file may be temporarily unavailable at the journal website or you do not have a PDF plug-in installed and enabled in your browser.

Alternatively, you can download the file locally and open with any standalone PDF reader:

https://link.springer.com/content/pdf/10.1186%2Fs11671-019-2947-5.pdf

Atomic Layer Deposition of Buffer Layers for the Growth of Vertically Aligned Carbon Nanotube Arrays

Nanoscale Research Letters December 2019, 14:119 | Cite as Atomic Layer Deposition of Buffer Layers for the Growth of Vertically Aligned Carbon Nanotube Arrays AuthorsAuthors and affiliations Hao-Hao LiGuang-Jie YuanBo ShanXiao-Xin ZhangHong-Ping MaYing-Zhong TianHong-Liang LuJohan Liu Open Access Nano Express First Online: 02 April 2019 73 Downloads Part of the following topical collections:Applications of Atomic Layer Deposition Abstract Vertically aligned carbon nanotube arrays (VACNTs) show a great potential for various applications, such as thermal interface materials (TIMs). Besides the thermally oxidized SiO2, atomic layer deposition (ALD) was also used to synthesize oxide buffer layers before the deposition of the catalyst, such as Al2O3, TiO2, and ZnO. The growth of VACNTs was found to be largely dependent on different oxide buffer layers, which generally prevented the diffusion of the catalyst into the substrate. Among them, the thickest and densest VACNTs could be achieved on Al2O3, and carbon nanotubes were mostly triple-walled. Besides, the deposition temperature was critical to the growth of VACNTs on Al2O3, and their growth rate obviously reduced above 650 °C, which might be related to the Ostwald ripening of the catalyst nanoparticles or subsurface diffusion of the catalyst. Furthermore, the VACNTs/graphene composite film was prepared as the thermal interface material. The VACNTs and graphene were proved to be the effective vertical and transverse heat transfer pathways in it, respectively. KeywordsAtomic layer deposition Vertically aligned carbon nanotube arrays Oxide buffer layers Thermal interface materials  Abbreviations ALD Atomic layer deposition C2H2 Acetylene CVD Chemical vapor deposition DEZ Diethylzinc DSC Differential scanning calorimeter EB Electron-beam FESEM Field emission scanning electron microscopy H2 Hydrogen LFA Laser flash thermal analyzer RBMs Radial breathing modes TDMAT Tetrakis(dimethylamino)titanium TEM Transmission electron microscopy TIMs Thermal interface materials TMA Trimethylaluminum VACNTs Vertically aligned carbon nanotubes Background Vertically aligned carbon nanotube arrays (VACNTs) have various outstanding performances and show great potential for a wide variety of applications. Due to their high axial thermal conductivity, many VACNT-based thermal interface materials (TIMs) have been developed for thermal packaging applications [1, 2, 3, 4, 5, 6, 7]. To synthesize the high-quality VACNTs on different substrates, chemical vapor deposition (CVD) has been commonly used, and the buffer layer should be deposited on the substrate before the deposition of the catalyst, such as Fe. Generally, the buffer layers are used to prevent the diffusion of the catalyst into substrates, so it is also very important to achieve the high-quality buffer layers on different substrates. Atomic layer deposition (ALD) has self-limited behavior, which could achieve pinhole-free, dense, and conformal films on complex non-planar substrates [8]. Recently, many researchers have used it to deposit the buffer layers for the growth of VACNTs [9, 10, 11]. Amama et al. reported the water-assisted CVD of VACNTs using ALD Al as the buffer layer [9]. Quinton et al. reported the floating catalyst CVD of VACNTs using Fe as the catalyst. They found that VACNTs had faster nucleation rate and more uniform tube diameter on ALD Al2O3 buffer layer, compared with SiO2 [10]. Compared with thermal and microwave plasma SiO2, the VACNTs grown on ALD SiO2 had the fastest nucleation rate [10]. Yang et al. reported that VACNTs could be synthesized on non-planar substrates using ALD Al2O3 as the buffer layer and Fe2O3 as the catalyst, respectively [11]. Compared with the planar surface, the non-planar surface could largely increase the specific surface area, which would be very beneficial for the preparation and further applications of VACNTs [12, 13, 14]. Although some ALD oxide buffer layers have been synthesized for the growth of VACNTs, their role was still not very clear in the CVD process. In this research, we used CVD to prepare the VACNTs with different buffer layers, including ALD Al2O3, ALD TiO2, ALD ZnO, and thermally oxidized SiO2. The effects of different oxide layers and deposition temperature on the growth of VACNTs were analyzed. Besides, the VACNTs/graphene composite film was also developed as the thermal interface material, and the VACNTs were used as the additional vertical thermal transfer pathways in it. Methods Al2O3, ZnO, and TiO2 thin films were deposited on Si substrates by ALD, and SiO2 was formed on Si substrate by thermal oxidization. Trimethylaluminum (TMA), tetrakis(dimethylamino)titanium (TDMAT), and diethylzinc (DEZ) were used as the precursors for ALD of Al2O3, TiO2, and ZnO films, respectively. For all of them, H2O was used as the oxygen source, and the deposition temperature was set at 200 °C. The thickness of Al2O3, ZnO, and TiO2, and SiO2 films was 20 nm. One-nanometer-thick Fe film was deposited on all of them by electron-beam (EB) evaporation, where it was used as the catalyst. The CVD method was applied to synthesize the VACNTs based on a commercial CVD system (AIXRON Black Magic II). Before the growth of VACNTs, the catalyst was annealed in the hydrogen (H2) atmosphere at 600 °C. The period was 3 min, and the flow rate of H2 was set at 700 sccm. After that, the acetylene (C2H2) and H2 were introduced into the chamber, and then VACNTs were prepared. The flow rates of C2H2 and H2 were 100 and 700 sccm, respectively. The deposition temperature was changed from 550 to 700 °C, and the period was fixed at 30 min. After the growth of VACNTs on Al2O3, the VACNTs/graphene composite film was also prepared as the thermal interface material. Epoxy resin, curing agent, and diluents were purchased from Sigma-Aldrich Trading and Tokyo Chemical Industrial Co., Ltd. The multilayer graphene was purchased from Nanjing Xianfeng Nanomaterials Technology Co., Ltd. For the preparation of the composite film, the catalyst was firstly patterned using a lithography machine (URE-2000S/A). The pattern size was 500 μm, and the distance was 150 μm among patterns. Secondly, the VACNTs were deposited by CVD at 650 °C, and the growth period was 30 min. Thirdly, the VACNTs were densified by the acetone vapor, and the period was 20 s. Fourthly, graphene, epoxy resin, curing agent, and diluent were mixed as the matrix, and the amount of graphene was fixed at 10 wt.%. After that, the VACNTs were immersed into the matrix and cured in a vacuum oven at 120 °C for 1 h and then at 150 °C for 1 h. Finally, the prepared composite film was polished to the thickness of about 300 μm, and the tips of VACNTs should be protruded from its both surfaces, as shown in Fig. 1. Open image in new window Fig. 1 Schematic diagram of the VACNTs/graphene composite film The morphology of VACNTs and the composite film was analyzed by the field emission scanning electron microscopy (FESEM, Merlin Compact) and transmission electron microscopy (TEM, Tecnai G2 F20 S-TWIN). Raman spectra of VACNTs were recorded by inVia Reflex, using a laser excitation wavelength of 632.8 nm. The thermal diffusivity (α) and specific heat capacity (Cp) of the composite film were measured by the laser flash thermal analyzer (Netzach LFA 467) and differential scanning calorimeter (DSC, Mettler Toledo DSC1), respectively. After that, the thermal conductivity could be calculated according to the Eq. 1: $$ \lambda =\alpha \times \mathrm{Cp}\times \rho, $$ (1) where λ and ρ were the thermal conductivity and density of the composite film, respectively. Results and Discussion Figure 2 a–d show the cross-sectional SEM images of VACNTs grown on different oxide buffer layers at 650 °C. The VACNTs have been successfully prepared on Al2O3, TiO2, and SiO2, as shown in Fig. 2 a, b, and d. Among them, the VACNTs were the thickest on Al2O3, which indicated that the lifetime of catalyst nanoparticles was the longest on it during the growth period. The lifetime of catalyst nanoparticles represents the time after it has basically lost its catalytic function to grow carbon nanotubes, which could be deduced from the thickness of VACNTs [9]. Unlike it, the relatively thin VACNTs were deposited on SiO2 and TiO2, which might be caused by the relatively serious Ostwald ripening of catalyst nanoparticles or the subsurface diffusion of Fe [15, 16]. As shown in Fig. 3, Ostwald ripening is a phenomenon whereby larger nanoparticles increase in size while smaller nanoparticles, which have greater strain energy, shrink in size and eventually disappear via atomic surface diffusion [17]. When a catalyst nanoparticle disappeared, or when too much catalyst was lost, the carbon nanotubes growing from it stopped [17]. Besides, subsurface diffusion of Fe into the buffer layer or substrate could also cause mass loss from the catalysts that grow the carbon nanotubes, eventually causing termination of growth [16]. From Fig. 2 a, b, and d, we could also see that the density of VACNTs was the highest on Al2O3, and the lowest on TiO2. Generally, any marginal alignment seen in CVD samples was due to a crowding effect, and carbon nanotubes supported each other by van der Waals attraction [18]. Therefore, it means that the density of VACNTS was quite important, and higher density generally resulted in better vertical alignment of VACNTs, which were confirmed in Fig. 2 a, b, and d. Besides, Fig. 2 c shows that there were almost no VACNTs grown on ZnO, which could be caused by much more serious Ostwald ripening of catalyst nanoparticles and subsurface diffusion of Fe, compared with others [15, 16]. Open image in new window Fig. 2 Cross-sectional SEM images of VACNTs grown on different oxide buffer layers at 650 °C: a Al2O3, b TiO2, c ZnO, and d SiO2 Open image in new window Fig. 3 Schematic illustration of Ostwald ripening and subsurface diffusion of Fe catalysts during the growth period of VACNTs Figure 4 a–d show Raman spectra of VACNTs grown on Al2O3, TiO2, ZnO, and SiO2. Generally, the D, G, and G’ bands were around 1360 cm−1, 1580 cm−1, and 2700 cm−1, respectively [19, 20]. For different oxide buffer layers, the ratio of ID and IG was calculated to be near or more than 1, and there were also no radial breathing modes (RBMs) around 200 cm−1. It indicated that all the prepared VACNTs were multi-walled on Al2O3, TiO2, ZnO, and SiO2. Figure 5 a–d show the morphology of VACNTs on different oxide buffer layers, which was analyzed by TEM. The VACNTs were multi-walled on all of them, which was consistent with the results of the Raman analysis. The VACNTs were mostly triple-walled on Al2O3, but more than four walls on TiO2, ZnO, and SiO2. Open image in new window Fig. 4 Raman spectra of VACNTs grown on different buffer layers at 650 °C: a Al2O3, b TiO2, c ZnO, and d SiO2. The spectra have been normalized to the intensity of the G band in order to facilitate comparison Open image in new window Fig. 5 TEM images of VACNTs grown on different buffer layers: a Al2O3, b TiO2, c ZnO, and d SiO2 Figure 6 shows the growth rate of VACNT variation with deposition temperature on Al2O3 and SiO2. When the temperature increased, the growth rate of VACNTs firstly raised and then decreased on both of them. It might be related to the serious Ostwald ripening of catalyst nanoparticles or subsurface diffusion of Fe, which largely reduced the lifetime of catalyst nanoparticles and the growth rate of VACNTs [15, 16]. Above 600 °C, the growth rate of VACNTs still increased on Al2O3, but decreased on SiO2. It indicated that the lifetime of catalyst nanoparticles on Al2O3 was longer than that on SiO2. When the deposition temperature was below 500 °C, there were obvious VACNTs on Al2O3 but no VACNTs on SiO2, which meant that the nucleation and initial growth of VACNTs were more easily achieved on Al2O3, compared with SiO2. It indicated that the activation energy for the nucleation and initial growth of VACNTs on Al2O3 was much lower than that on SiO2. Commonly, each catalyst nanoparticle could produce at most one carbon nanotube, but not all the catalyst nanoparticles could achieve the carbon nanotubes, because the activation energy should be overcome for their nucleation and initial growth [21, 22, 23]. Therefore, compared with SiO2, the lower activation energy of VACNTs on Al2O3 might result in their higher density, which could be confirmed by Fig. 2 a and d. Open image in new window Fig. 6 The growth rate of VACNTs variation with deposition temperature on Al2O3 and SiO2 buffer layers Figure 7 a shows the morphology of VACNTs with the patterned catalyst on Al2O3. Generally, there still had a lot of gaps inside VACNTs, which were filled with air, as shown in Fig. 2 a. However, the thermal conductivity of air was only 0.023 Wm−1 K−1 at room temperature, so the VACNTs need to be densified to remove it. From Fig. 7 b, we could see that the obvious densification of VACNTs has been achieved with the acetone vapor. Figure 7 c shows the cross-sectional image of the VACNTs/graphene composite film. The VACNTs and graphene were used as the additional vertical and transverse thermal transfer pathways in it. Figure 8 a and b show the vertical and transverse thermal conductivities of the composite film, which were measured to be about 1.25 and 2.50 Wm−1 K−1, respectively. Compared with the pure epoxy resin, its vertical and transverse thermal conductivities have been obviously enhanced. It confirmed that the effective vertical and transverse heat transfer pathways have been offered by the VACNTs and graphene in the composite film, respectively. Open image in new window Fig. 7 a The SEM image of VACNTs with the patterned catalyst. b The SEM image of VACNTs after the densification. c The cross-sectional SEM image of the VACNTs/graphene composite film Open image in new window Fig. 8 Thermal property of the VACNTs/graphene composite film: a the vertical thermal conductivity and b the transverse thermal conductivity Conclusions The growth of VACNTs has been analyzed on different oxide buffer layers, such as ALD Al2O3, ALD TiO2, ALD ZnO, and thermally oxidized SiO2. Among them, VACNTs were the thickest and densest on Al2O3, which indicated that the lifetime of catalyst nanoparticles was the longest and the vertical alignment of VACNTs was the best on it. Besides, the VACNTs were found to be multilayer on Al2O3, and the deposition temperature was very critical to the growth of VACNTs. Compared with SiO2, the nucleation and initial growth of VACNTs were more easily achieved on Al2O3, which resulted in a higher density of VACNTs on it. After the growth of VACNTs on Al2O3, they were used to prepare the composite film together with graphene and epoxy resin. Compared with the pure epoxy resin, the vertical and transverse thermal conductivities of the composite film have been largely improved. Notes Acknowledgements The authors thank Dr. Yong Zhang from the School of Automation and Mechanical Engineering, Shanghai University, for the useful discussions. Funding This work was financially supported by the National Natural Science Foundation of China (Nos. 61704102 and 51861135105). Availability of Data and Materials The datasets supporting the conclusions of this article are included with the article. Authors’ Contributions HHL, GJY, BS, XXZ, and HPM designed the experiments and analyzed the data. HHL, GJY, BS, XXZ, HPM, YZT, HLL, and JL discussed the results and contributed to the writing of the manuscript. All authors read and approved the final manuscript. Competing Interests The authors declare that they have no competing interests. Publisher’s Note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations. References 1. Li L, Yang Z, Gao H, Zhang H, Ren J, Sun X, Chen T, Kia HC, Peng H (2011) Vertically aligned and penetrated carbon nanotube/polymer composite film and promising electronic applications. Adv Mater. 23:3730–3735CrossRefGoogle Scholar 2. Wang CY, Chen TH, Chang SC, Cheng SY, Chin TS (2010) Strong carbon-nanotube-polymer bonding by microwave irradiation. Adv Funct Mater. 17:1979–1983CrossRefGoogle Scholar 3. Peacock MA, Roy CK, Hamilton MC, Johnson RW, Knight RW, Harris DK (2016) Characterization of transferred vertically aligned carbon nanotubes arrays as thermal interface materials. Int J Heat Mass Tran. 97:94–100CrossRefGoogle Scholar 4. Ping LQ, Hou PX, Liu C, Li JC, Zhao Y, Zhang F, Ma CQ, Tai KP, Cong HT, Cheng HM (2017) Surface-restrained growth of vertically aligned carbon nanotube arrays with excellent thermal transport performance. Nanoscale 9:8213–8219CrossRefGoogle Scholar 5. Hao ML, Huang ZX, Saviers KR, Xiong GP, Hodson SL, Fisher TS (2017) Characterization of vertically oriented carbon nanotubes arrays as high-temperature thermal interface materials. Int J Heat Mass Tran. 106:1287–1293CrossRefGoogle Scholar 6. Uetani K, Ata S, Tomonoh S, Yamada T, Yumura M, Hata K (2014) Elastomeric thermal interface materials with high through-plane thermal conductivity from carbon fiber fillers vertically aligned by electrostatic flocking. Adv Mater. 26:5857–5862CrossRefGoogle Scholar 7. Wang M, Li TT, Yao YG, Lu HF, Li Q, Chen MH, Li QW (2014) Wafer-scale transfer of vertically aligned carbon nanotube arrays. J Am Chem Soc. 136:18156–18162CrossRefGoogle Scholar 8. George SM (2010) Atomic layer deposition: an overview. Chem Rev. 110:111–131CrossRefGoogle Scholar 9. Amama PB, Pint CL, Kim SM, Mcjilton L, Eyink KG, Stach EA, Hauge RH, Maruyama B (2010) Influence of alumina type on the evolution and activity of alumina-supported Fe catalysts in single-walled carbon nanotube carpet growth. Acs Nano 4:895–904CrossRefGoogle Scholar 10. Quinton BT, Leedy KD, Lawson JW, Tsao B, Scofield JD, Merrett JN, Zhang Q, Yost K, Mukhopadhyay SM (2015) Influence of oxide buffer layers on the growth of carbon nanotube arrays on carbon substrates. Carbon 87:175–185CrossRefGoogle Scholar 11. Yang C, Li Y, Yan L, Cao YZ (2016) Influence of catalyst film thickness deposited by atomic layer deposition on growth of aligned carbon nanotubes. J Inorg Mater. 31:681–686CrossRefGoogle Scholar 12. Zhang Q, Huang JQ, Zhao MQ, Qian WZ, Wang Y, Wei F (2008) Radial growth of vertically aligned carbon nanotube arrays from ethylene on ceramic spheres. Carbon 46:1152–1158CrossRefGoogle Scholar 13. Zhou K, Huang JQ, Zhang Q, Wei F (2010) Multi-directional growth of aligned carbon nanotubes over catalyst film prepared by atomic layer deposition. Nanoscale Res Lett. 5:1555–1560CrossRefGoogle Scholar 14. Xiang R, Luo GH, Qian WZ, Wang Y, Wei F, Li Q (2007) Large area growth of aligned CNT arrays on spheres: towards large scale and continuous production. Chem Vapor Depos. 13:533–536CrossRefGoogle Scholar 15. Navas H, Picher M, Ledier AA, Fossard F, Michel T, Kozawa A, Maruyama T, Anglaret E, Loiseau A, Jourdain V (2017) Unveiling the evolutions of nanotube diameter distribution during the growth of single-walled carbon nanotubes. ACS Nano 11:3081–3088CrossRefGoogle Scholar 16. Kim SM, Pint CL, Amama PB, Zakharov DN, Hauge RH, Maruyama B, Stach EA (2010) Evolution in catalyst morphology leads to carbon nanotube growth termination. J Phys Chem Lett. 1:918–922CrossRefGoogle Scholar 17. Amama PB, Pint CL, McJilton L, Kim SM, Stach EA, Murray PT, Hauge RH, Maruyam B (2009) Role of water in super growth of single-walled carbon nanotube carpets. Nano Lett. 9:44–49CrossRefGoogle Scholar 18. Lee IH, Han GH, Chae SJ, Bae JJ, Kim ES, Kim SM, Kim TH, Jeong HK, Lee YH (2010) Criteria for producing yarns from vertically aligned carbon nanotubes. Nano 5:31–38CrossRefGoogle Scholar 19. Kuznetsov VL, Bokova-Sirosh SN, Moseenkov SI, Ishchenko AV, Krasnikov DV, Kazakova MA, Romanenko AI, Tkachev EN, Obraztsova ED (2014) Raman spectra for characterization of defective CVD multi-walled carbon nanotubes. Phys Status Solidi B 251:2444–2450CrossRefGoogle Scholar 20. Delosarcos T, Garnier MG, Oelhafen P, Mathys D, Seo JW, Domingo C, Vicente Garcia RJ, Sanchez CS (2004) Strong influence of buffer layer type on carbon nanotube characteristics. Carbon 42:187–190CrossRefGoogle Scholar 21. Kharlamova MV (2017) Investigation of growth dynamics of carbon nanotubes. Beilstein J Nanotechnol. 8:826–856CrossRefGoogle Scholar 22. In JB, Grigoropoulos CP, Chernov AA, Noy A (2011) Growth kinetics of vertically aligned carbon nanotube arrays in clean oxygen-free condition. ACS Nano 5:9602–9610CrossRefGoogle Scholar 23. Chen GH, Davis RC, Kimura H, Sakurai S, Yumura M, Futaba DN, Hata K (2015) The relationship between the growth rate and the lifetime in carbon nanotube synthesis. Nanoscale 7:8873–8878CrossRefGoogle Scholar Copyright information © The Author(s). 2019 Open AccessThis article is distributed under the terms of the Creative Commons Attribution 4.0 International License (http://creativecommons.org/licenses/by/4.0/), which permits unrestricted use, distribution, and reproduction in any medium, provided you give appropriate credit to the original author(s) and the source, provide a link to the Creative Commons license, and indicate if changes were made. Authors and Affiliations Hao-Hao Li1Guang-Jie Yuan1Email authorBo Shan1Xiao-Xin Zhang1Hong-Ping Ma2Ying-Zhong Tian3Hong-Liang Lu2Johan Liu141.SMIT Center, School of Automation and Mechanical EngineeringShanghai UniversityShanghaiPeople’s Republic of China2.State Key Laboratory of ASIC and System, School of MicroelectronicsFudan UniversityShanghaiPeople’s Republic of China3.Shanghai Key Laboratory of Intelligent Manufacturing and Robotics, School of Automation and Mechanical EngineeringShanghai UniversityShanghaiPeople’s Republic of China4.Electronics Materials and Systems Laboratory, Department of Microtechnology and NanoscienceChalmers University of TechnologyGoteborgSweden


This is a preview of a remote PDF: https://link.springer.com/content/pdf/10.1186%2Fs11671-019-2947-5.pdf

Hao-Hao Li, Guang-Jie Yuan, Bo Shan, Xiao-Xin Zhang, Hong-Ping Ma, Ying-Zhong Tian, Hong-Liang Lu, Johan Liu. Atomic Layer Deposition of Buffer Layers for the Growth of Vertically Aligned Carbon Nanotube Arrays, Nanoscale Research Letters, 2019, 119, DOI: 10.1186/s11671-019-2947-5